At a glance
- Under ASTM D5336-22, polyphthalamide (PPA) is a polyamide whose acid component is at least 55 mol % terephthalic or isophthalic acid.
- Pure PA6T melts at 370 °C, above its decomposition temperature; copolymers with melting points below 330 °C are processed.
- PA9T melts at about 308 °C, PA10T at about 316 to 318 °C; PA66 is below 260 °C.
- Water absorption is lower than for PA66, but moist parts made of PA6T copolymers can still blister during reflow soldering.
- Values are only comparable with the standard: ISO 62 (water absorption), ISO 75-2 (heat deflection temperature), IEC 60216 and UL 746B (continuous temperature).
PPA: definition and abbreviations
What is a polyphthalamide?
A polyphthalamide (PPA) is a polyamide in which terephthalic acid, isophthalic acid or both together make up at least 55 mol % of the dicarboxylic acid component of the chain. This is how ASTM D5336 defines it, the classification system for PPA injection moulding materials, currently in the 2022 version.[1] The diamine is aliphatic, usually hexamethylenediamine. The aromatic rings in the chain raise the melting and glass transition temperatures compared with PA6 and PA66.[11] The term semi-aromatic polyamides is also common.[9]
A technical review groups as high-temperature polyamides the semi-crystalline grades with a melting point above 280 °C, in industry also from 270 °C. According to it, the commercial series are PA46, PA6T, PA9T and PA10T.[9] PA46 is aliphatic and not a PPA.
How do you read abbreviations such as PA6T/66?
The digit stands for the number of carbon atoms in the diamine, T for terephthalic acid and I for isophthalic acid; the slash separates the building blocks of a copolymer. PA6T/6I therefore contains hexamethylenediamine with both acids, PA6T/66 adipic acid in addition.[9][11] The abbreviations of the basic polymers are set by ISO 1043-1:2011, the designation of polyamide moulding materials by ISO 16396-1:2022. This designation contains no design data.[2][3]
The texts of the standards are subject to a charge and were not available to the editors. The information comes from public abstracts and previews. The text of the standard is authoritative.
| Abbreviation | Structure | Melting point | Glass transition, note |
|---|---|---|---|
| PA6T | hexamethylenediamine and terephthalic acid | 370 °C | decomposition from about 350 °C |
| PA6T/66 | plus adipic acid | 308 to 325 °C | 88 to 100 °C |
| PA6T/6I | plus isophthalic acid | 319 to 325 °C | 125 to 135 °C |
| PA6/6T (PA6T/6) | plus caprolactam | 298 °C | 125 °C (one grade) |
| PA9T | nonanediamine and terephthalic acid | 300 to 308 °C | 125 °C |
| PA10T | decanediamine and terephthalic acid | 316 to 318 °C | 115 to 120 °C |
| PA66 (comparison) | aliphatic | below 260 °C | not a PPA |
PA9T and PA10T: longer diamines
What distinguishes PA9T from PA6T?
PA9T is made from terephthalic acid and a diamine with nine carbon atoms and therefore contains fewer amide groups per chain length than PA6T. The lower amide concentration leads to lower water absorption.[9] Pure PA9T melts at about 308 °C. Usually a branched isomer of the diamine is copolymerised at less than 20 mol %, which lowers the melting point.[9]
The high share of methylene groups makes PA9T crystallise quickly.[9]
PA10T, from terephthalic acid and decanediamine, melts at about 316 to 318 °C and, according to the review, has the lowest water absorption of the industrially produced high-temperature polyamides.[9][10] The decanediamine is obtained from castor oil. The polymer gradually decomposes from about 340 °C, which limits the processing temperature.[9] A patent names very fast crystallisation as a drawback: the melt can freeze in the nozzle.[12]
PA6/6T and other PA6T copolymers
Why is PA6T only available as a copolymer?
Pure PA6T melts at 370 °C and already decomposes from about 350 °C. It therefore cannot be processed from the melt.[9] Copolymers with a melting point below 330 °C are used technically. Common comonomers are adipic acid (PA6T/66), isophthalic acid (PA6T/6I), caprolactam (PA6/6T, also written PA6T/6) and 2-methylpentanediamine. Because of its low cost, the PA6T series is the most widespread group.[9]
The comonomer determines melting point, glass transition and crystallinity. Adipic acid can replace terephthalic acid in the crystal; all PA6T/66 copolymers melt higher than PA66.[9] Isophthalic acid disrupts crystallisation. In a study on PA6I/6T, the copolymer with 70 % 6I content was amorphous. With 70 % 6T content it melted at 319 °C, at a crystallinity of 16.4 %. The glass transition temperature was around 130 °C in all cases.[11]
Properties, applications and limits
How much water do semi-aromatic polyamides absorb?
Semi-aromatic polyamides absorb less water than PA6 and PA66, for which a patent gives up to about 10 %. For PA6T copolymers, absorption is nevertheless enough to make precision parts swell.[12] For PA10T, a measurement to ISO 62 with water immersion to saturation gave 2.48 %.[10] Such figures are only comparable with the same method and the same immersion time.[4]
| Property | Standard and edition | Content |
|---|---|---|
| Water absorption | ISO 62:2008 | exposure to water or humid air |
| Heat deflection temperature | ISO 75-2:2013 | methods A, B, C with 1.80, 0.45 and 8.00 MPa |
| Temperature index | IEC 60216-1:2025 | ageing, Arrhenius evaluation |
| Relative Thermal Index | UL 746B, 5th edition 2018 | long-term tests, revised several times since |
| Solderability of components | J-STD-020F (2022) | moisture and reflow sensitivity |
Which temperatures can they withstand?
For short-term loading, the review gives heat deflection temperatures above 260 °C for high-temperature polyamides, without stating test stress and reinforcement.[9] ISO 75-2 has three flexural stresses; the value only applies together with the method.[5] The continuous temperature is determined by oven ageing, as a temperature index to IEC 60216 or as a Relative Thermal Index (RTI) to UL 746B. Under UL 746B the samples are aged at at least four temperatures, the longest series over at least 5,000 hours.[6][7]
Are they suitable for lead-free reflow soldering?
Yes, but moisture in the part also decides. Lead-free solders require temperatures above 250 °C; in reflow soldering up to 270 °C occur.[9] If absorbed water evaporates inside the part, blisters form (blistering). For PA6T copolymers this is to be expected without proper drying. In the comparison reproduced there, PA9T remained free of blisters.[9] The temperature profile and moisture sensitivity levels for components are described in J-STD-020F.[8]
How resistant are they to media?
PPA are chemically more resistant than aliphatic polyamides, but the grades differ markedly.[11] In a comparison in the review, PA9T retained 90 % of its tensile strength after seven days in water at 80 °C, PA6T 63 %. In methanol the figures were 72 and 35 %.[9] These are individual values.
What must be considered in processing?
Processing requires high melt temperatures. PA6I/6T with 70 % 6T content was moulded at a barrel temperature of 330 °C.[11] A study on PA10T worked with 310 to 330 °C at the barrel and a mould temperature of 150 °C, after eight hours of drying at 120 °C.[10] A patent states that older polyphthalamides need mould temperatures that water-heated moulds cannot reach.[12]
Where are high-temperature polyamides used?
- Electronics: connectors for surface mounting, circuit breakers.[9]
- Automotive: engine and powertrain parts, thermostat housings, charge air coolers.[9]
- Lighting: carriers and reflectors for light-emitting diodes.[9]
What are they not suited for?
- Precision parts in humid environments: PA6T copolymers swell too much for this.[12]
- Contact with alcohols: PA6T lost around two thirds of its tensile strength in methanol.[9]
What the material supplier needs to know
- Continuous temperature and temperature peaks, with duration of exposure
- Soldering method and peak temperature, if the part is soldered
- Contact media with concentration and temperature
- Permissible dimensional change due to moisture
- Mechanical requirements at service temperature
- Required flammability rating and required temperature index
- Wall thickness, flow path and available mould temperature control
- Standards to which the properties are to be demonstrated
Frequently asked questions
What is PPA?
PPA stands for polyphthalamide. Under ASTM D5336, at least 55 mol % of its dicarboxylic acid component consists of terephthalic or isophthalic acid.
What is the difference between PPA and PA66?
PA66 is purely aliphatic and melts below 260 °C. PPA contains aromatic acid building blocks, melts higher and absorbs less water.
Why is PA6T not processed as a pure polymer?
Pure PA6T melts at 370 °C and already decomposes from about 350 °C. Copolymers such as PA6T/66 or PA6T/6I are therefore processed.
What is the melting point of PA9T?
According to the technical literature, pure PA9T melts at about 308 °C, a grade with comonomer at 300 °C.
What does the T in PA6T mean?
The T stands for terephthalic acid, the digit before it for the carbon atoms in the diamine. An I stands for isophthalic acid.
Is PA9T a polyphthalamide?
Yes. The acid component of PA9T is terephthalic acid, so it meets the definition under ASTM D5336, as does PA10T.
Why do polyamide parts blister during reflow soldering?
Absorbed water evaporates inside the part at soldering temperatures above 250 °C. Without drying, PA6T copolymers are more at risk than PA9T.
What is the difference between heat deflection temperature and temperature index?
The heat deflection temperature to ISO 75 is a short-term value under flexural load. The temperature index describes ageing over thousands of hours.
Is PA10T bio-based?
Partly. The diamine of PA10T, decanediamine, is obtained from castor oil.
Sources
All sources retrieved and checked on 23 November 2026.
- ASTM D5336-22, Standard Classification System and Basis for Specification for Polyphthalamide (PPA) Injection Molding Materials. Abstract and preview. https://store.astm.org/d5336-22.html
- ISO 16396-1:2022, Plastics – Polyamide (PA) moulding and extrusion materials – Part 1: Designation system and basis for specifications. 2nd edition, September 2022. Abstract. https://www.iso.org/standard/81940.html
- ISO 1043-1:2011, Plastics – Symbols and abbreviated terms – Part 1: Basic polymers and their special characteristics. 4th edition, with Amendment 1:2016, confirmed 2022. Abstract. https://www.iso.org/standard/50590.html
- ISO 62:2008, Plastics – Determination of water absorption. 3rd edition, confirmed 2021. Abstract. https://www.iso.org/standard/41672.html
- ISO 75-2:2013, Plastics – Determination of temperature of deflection under load – Part 2: Plastics and ebonite. 3rd edition, confirmed 2025. Abstract. https://www.iso.org/standard/55653.html
- IEC 60216-1:2025, Electrical insulating materials – Thermal endurance properties – Part 1: Ageing procedures and evaluation of test results. 7th edition, December 2025. Abstract. https://webstore.iec.ch/en/publication/110870
- UL 746B, Polymeric Materials – Long Term Property Evaluations, 5th edition 2018. Notice from a test laboratory on the revision of 2 August 2019 with details of the ageing programme. https://cdn.intertek.com/www-intertek-com/dms-legacy/UL-746B-Rev-8-2-2019-ED-12-6-2021.pdf
- IPC/JEDEC J-STD-020F, Moisture/Reflow Sensitivity Classification for Non-hermetic Surface Mount Devices (SMDs). December 2022. Abstract. https://www.dinmedia.de/en/standard/ipc-jedec-j-std-020f/366816203
- Zhang, C.: Progress in semicrystalline heat-resistant polyamides. e-Polymers 18 (2018), no. 5, pp. 373–408. https://doi.org/10.1515/epoly-2018-0094
- Xia, H.; Jiang, Z.; Tang, J.; Tang, J.; Zhou, J.; Yang, Z.; Zheng, R.; Niu, J.: Preparation and Properties of PA10T/PPO Blends Compatibilized with SEBS-g-MAH. Polymers 16 (2024), 1598. https://doi.org/10.3390/polym16111598
- Djukic, S.; Bocahut, A.; Bikard, J.; Long, D. R.: Mechanical properties of amorphous and semi-crystalline semi-aromatic polyamides. Heliyon 6 (2020), e03857. https://doi.org/10.1016/j.heliyon.2020.e03857
- US Patent 7,927,710: Semiaromatic polyamide molding compositions and their use. Background section. https://image-ppubs.uspto.gov/dirsearch-public/print/downloadPdf/7927710
Related topics
- PPS and PEEK
Chemical resistance, fire behaviour and continuous use temperature. - Metal replacement
Stiffness, creep and temperature: when a plastic can replace a metal part. - Halogen-free flame retardancy
UL 94, Yellow Card and glow-wire tests: what the classes mean and how they are demonstrated. - Thermally conductive plastics
The value in W/(m·K), test methods, electrically insulating or conductive, applications and limits.
This page is technical information, not advice on standards, law or design. The standards cited in their current edition and the material manufacturers' test reports are authoritative.