Skip to content
Spezialcompounds Reference guide to engineering plastic compounds Deutsch

Electrically conductive plastics

Electrically conductive plastics are thermoplastics that dissipate charge through conductive carbon black, carbon fibres, carbon nanotubes, graphite or metal. The German technical rule TRGS 727 calls a material conductive up to 10⁴ Ωm volume resistivity and dissipative between 10⁴ and 10⁹ Ωm. Testing follows IEC 62631-3-1, IEC 62631-3-2 or ISO 3915.

Last reviewed:

At a glance

  • TRGS 727 distinguishes conductive, dissipative and insulating and gives resistance limits for each.
  • Surface resistance depends on humidity, so the test atmosphere belongs with every value.
  • ESD protection in electronics manufacturing is governed by IEC 61340-5-1:2024, explosion protection of equipment by IEC 60079-0:2026.
  • Conductivity only appears above the percolation threshold, where the filler particles form continuous paths.
  • Near the percolation threshold, injection moulding conditions change the resistance by several orders of magnitude.

Resistance ranges: insulating, dissipative, conductive

When is a plastic considered conductive or dissipative?

Under the German technical rule TRGS 727, a material is conductive if its volume resistivity is at most 104 Ωm, and dissipative if it lies between 104 and 109 Ωm. Everything else is considered insulating. For objects, the rule also gives limits for surface resistance, depending on the test atmosphere.⁠[9] Unfilled plastics lie far within the insulating range.⁠[10]

Resistance ranges conductive, dissipative, insulating under TRGS 727conductive: up to 10⁴; dissipative: 10⁴ to 10⁹; insulating: from 10⁹ (Ω·m).conductiveup to 10⁴dissipative10⁴ to 10⁹insulatingfrom 10⁹110⁴10⁹10¹²Ω·m, logarithmic
Classification by volume resistivity under TRGS 727. Separate limits apply to surface resistance, see table. The limits of the ESD standards are not shown. Source: [9].

What distinguishes surface and volume resistance?

Volume resistance is measured through the material, surface resistance on the surface of an object. Related to unit length and unit cross-section, this gives the resistivity in Ωm. For surface resistance, TRGS 727 describes two parallel electrodes 100 mm long and 10 mm apart.⁠[9]

Which standards govern the measurement?

For insulating materials, IEC 62631-3-1 (volume resistance) and IEC 62631-3-2 (surface resistance) apply, both with direct voltage and both in their second edition of 2023.⁠[1]⁠[2] For plastics made conductive there is ISO 3915, second edition of February 2022. It applies to materials with a resistivity below 106 Ω·cm, which corresponds to 104 Ω·m.⁠[3]

Classification under TRGS 727 and matching test standards
Class under TRGS 727Volume resistivitySurface resistanceMatching test standard and edition
conductiveat most 10⁴ Ωmat most 10⁴ ΩISO 3915:2022
dissipativeabove 10⁴ and below 10⁹ Ωm10⁴ to 10⁹ Ω at 23 °C and 50 % relative humidity; 10⁴ to 10¹¹ Ω at 30 %IEC 62631-3-1:2023 (volume), IEC 62631-3-2:2023 (surface)
insulatingabove thatabove thatas dissipative
Sources: terms and values after TRGS 727 [9]; standards after the abstracts [1], [2], [3]. The assignment of test standards is not a requirement of TRGS 727.

The texts of the standards are subject to a charge and were not available to the editors. The information comes from the public abstracts of the issuing bodies; for TRGS 727 and Directive 2014/34/EU from the full text.

ESD: protecting electronic devices

What does ESD protection in electronics manufacturing require?

IEC 61340-5-1 sets the organisational and technical requirements for an ESD control programme. ESD stands for electrostatic discharge. The current edition is the third of May 2024; it replaces the 2016 edition.⁠[4]

The standard covers devices that withstand at least 100 V under the human body model and 200 V under the charged device model. Requirements for packaging are in a separate part of the series, IEC 61340-5-3.⁠[4]

Do the ESD standards also apply to explosion protection?

No. IEC 61340-5-1 expressly excludes flammable liquids, gases and dusts.⁠[4] The resistance limits of the ESD standards are not publicly accessible and are therefore not given here.

ATEX: charging in potentially explosive atmospheres

What do the ATEX Directive and IEC 60079-0 require?

Directive 2014/34/EU requires the manufacturer to prevent, by suitable measures, electrostatic charges capable of causing dangerous discharges (Annex II, point 1.3.2). It has applied since 20 April 2016.⁠[8]

How this is implemented for equipment is governed by IEC 60079-0. The eighth edition was published on 16 June 2026 and replaces the 2017 edition. A separate clause deals with electrostatic charges on external non-metallic parts. As tests, the table of contents names the measurement of surface resistance and of transferred charge.⁠[6] The limit values are in the text of the standard. IEC TS 60079-32-1 of 2013, amended 2017, supplements it as guidance.⁠[7]

Which values does TRGS 727 give?

TRGS 727 requires that, in potentially explosive atmospheres, only conductive or dissipative objects are used in principle. Conductive objects must be earthed; dissipative ones need contact to earth. If a part remains insulating, the rule limits its surface area: in zone 1 to 100 cm² for explosion groups IIA and IIB and to 20 cm² for IIC, in zone 0 to 50, 25 and 4 cm².⁠[9] The rule applies in the edition of January 2016.⁠[9]

Humidity can lower surface resistance, but this does not make plastics such as PTFE or PE dissipative.⁠[9]

Fillers, applications and limits

What is the percolation threshold?

The percolation threshold is the filler content at which the conductive particles form continuous paths. Above it, conductivity rises by several orders of magnitude.⁠[11] Fillers with a high ratio of length to diameter reach it earlier than carbon black.⁠[10]⁠[11]

Conductive fillers and additives
FillerFigure from the literatureNote
Conductive carbon blackpercolation at about 5 to 15 % by volumehigh filler content needed
Carbon nanotubespercolation at about 0.1 to 3 % by volumereacts strongly to processing
Carbon fibresalignment in injection moulding lowered the threshold in one studyprocessing determines the result
Graphiteexpanded graphite in PMMA: 0.29 % by volumesingle example
Metal fibres and metal powderpowder: percolation at around 10 to 30 % by volumecost, oxide layers
Permanent antistatic polymerABS with 20 % additive: about 10¹⁰ ohmindependent of humidity
Sources: [5], [10], [11], [12]. Research examples, not a market overview.

What do permanent antistatic additives achieve?

Permanent antistatic additives are polymers that do not migrate to the surface and work independently of humidity. A patent describes block copolymers of polyamide blocks and hydrophilic blocks for this. According to it, conventional antistatic agents are ionic surfactants whose effect depends on humidity and is lost over time. In the patent's example, the surface resistance of ABS with 20 % additive fell from 1014 to about 1010 ohm.⁠[12]

Where are conductive plastics used?

  • Electronics manufacturing: handling, packaging and transport of devices sensitive to electrostatic discharge.⁠[4]
  • Chemicals and bulk handling: pipes and hoses for bulk materials in potentially explosive atmospheres.⁠[9]
  • Equipment for hazardous areas: housings and external parts made of non-metallic materials.⁠[6]
  • Electromagnetic shielding: protection of electronic components.⁠[11]

Where are the limits?

The resistance of a part can differ markedly from that of the test specimen.

  • Processing: in polypropylene with carbon nanotubes, a higher mould temperature and a higher injection rate lowered the resistance by several orders of magnitude.⁠[5]
  • Direction: in the same study, the percolation threshold was lower in-plane than through the thickness.⁠[5]
  • Mechanics: filler contents above the threshold can embrittle the material and raise the melt viscosity.⁠[11]
  • Metallic fillers: they are expensive and form oxide layers.⁠[11]

What the material supplier needs to know

  • Target resistance range: surface or volume resistance, with upper and lower limit
  • Test standard, test voltage and test atmosphere (temperature and relative humidity)
  • Rules for the application: ESD protection to IEC 61340-5-1 or explosion protection to IEC 60079-0 and TRGS 727
  • For hazardous areas: zone, explosion group and size of the plastic surface
  • Earthing concept of the part
  • Wall thickness, flow path and processing method
  • Required colour
  • Mechanical requirements
  • Temperature, humidity and media contact in service

Frequently asked questions

What is an electrically conductive plastic?

An electrically conductive plastic is a thermoplastic that dissipates charge through fillers such as conductive carbon black, carbon fibres or graphite. Unfilled plastics are insulators.

What is the difference between conductive and dissipative?

Under TRGS 727, a material is conductive up to a volume resistivity of 10⁴ Ωm. It is dissipative between 10⁴ and 10⁹ Ωm; above that it is considered insulating.

Which standard applies to measuring surface resistance?

IEC 62631-3-2:2023 describes the measurement with direct voltage. For volume resistance, IEC 62631-3-1:2023 applies, and for conductive plastics ISO 3915:2022.

What is an ESD compound?

An ESD compound is a plastic for protecting electronic devices against electrostatic discharge. The requirements for the ESD control programme are in IEC 61340-5-1:2024, those for packaging in IEC 61340-5-3.

Which plastic is permitted in ATEX areas?

TRGS 727 requires, in principle, conductive or dissipative objects with earthing or contact to earth in potentially explosive atmospheres. Insulating surfaces are limited in size depending on zone and explosion group.

How large may an insulating plastic surface be in zone 1?

TRGS 727 gives at most 100 cm² for zone 1 in explosion groups IIA and IIB and at most 20 cm² in IIC. In zone 0 the values are 50, 25 and 4 cm².

What is the percolation threshold?

The percolation threshold is the filler content at which conductive particles form continuous paths in the plastic. Above it, conductivity rises by several orders of magnitude.

Why does the resistance of a part differ from the data sheet?

In a study on polypropylene with carbon nanotubes, mould temperature and injection rate shifted the resistance by several orders of magnitude.

What is a permanent antistatic plastic?

A permanent antistatic plastic contains a polymeric additive that does not migrate to the surface. Unlike ionic surfactants, it works independently of humidity.

Sources

All sources retrieved and checked on 23 November 2026.

  1. IEC 62631-3-1:2023, Dielectric and resistive properties of solid insulating materials – Part 3-1: Determination of resistive properties (DC methods) – Volume resistance and volume resistivity. 2nd edition, January 2023. Abstract. https://webstore.iec.ch/publication/62314
  2. IEC 62631-3-2:2023, Part 3-2: Determination of resistive properties (DC methods) – Surface resistance and surface resistivity. 2nd edition, October 2023. Abstract. https://webstore.iec.ch/publication/62315
  3. ISO 3915:2022, Plastics – Measurement of resistivity of conductive plastics. 2nd edition, February 2022. Abstract. https://www.iso.org/standard/81838.html
  4. IEC 61340-5-1:2024, Electrostatics – Part 5-1: Protection of electronic devices from electrostatic phenomena – General requirements. 3rd edition, May 2024. Abstract and preview. https://webstore.iec.ch/publication/74748
  5. Zaccone, M.; Armentano, I.; Cesano, F.; Scarano, D.; Frache, A.; Torre, L.; Monti, M.: Effect of Injection Molding Conditions on Crystalline Structure and Electrical Resistivity of PP/MWCNT Nanocomposites. Polymers 12 (2020), 1685. https://doi.org/10.3390/polym12081685
  6. IEC 60079-0:2026, Explosive atmospheres – Part 0: Equipment – General requirements. 8th edition, June 2026. Abstract and preview (table of contents, foreword). https://webstore.iec.ch/en/publication/71519
  7. IEC TS 60079-32-1:2013 with Amendment 1:2017, Explosive atmospheres – Part 32-1: Electrostatic hazards, guidance. Abstract. https://webstore.iec.ch/publication/651
  8. Directive 2014/34/EU of the European Parliament and of the Council of 26 February 2014 on equipment and protective systems intended for use in potentially explosive atmospheres (recast). Full text. https://eur-lex.europa.eu/legal-content/EN/TXT/?uri=CELEX:32014L0034
  9. TRGS 727, Vermeidung von Zündgefahren infolge elektrostatischer Aufladungen (German technical rule: avoiding ignition hazards from electrostatic charges). Edition January 2016, GMBl 2016 p. 256, corrected p. 623. Full text. https://vorschriften.bgn-branchenwissen.de/daten/tr/trgs727/titel.htm
  10. Huang, Y.; Ellingford, C.; Bowen, C.; McNally, T.; Wu, D.; Wan, C.: Tailoring the electrical and thermal conductivity of multi-component and multi-phase polymer composites. International Materials Reviews (2019). https://doi.org/10.1080/09506608.2019.1582180
  11. Nan, X.; Zhang, Y.; Shen, J.; Liang, R.; Wang, J.; Jia, L.; Yang, X.; Yu, W.; Zhang, Z.: A Review of the Establishment of Effective Conductive Pathways of Conductive Polymer Composites and Advances in Electromagnetic Shielding. Polymers 16 (2024), 2539. https://doi.org/10.3390/polym16172539
  12. US Patent 9,957,386: Antistatic thermoplastic starch alloys. Background section and examples. https://patents.google.com/patent/US9957386B2/en

Related topics

  • Thermally conductive plastics
    The value in W/(m·K), test methods, electrically insulating or conductive, applications and limits.
  • Colour
    Colour matching, colour systems, colour difference and laser marking.
  • Halogen-free flame retardancy
    UL 94, Yellow Card and glow-wire tests: what the classes mean and how they are demonstrated.
  • Metal replacement
    Stiffness, creep and temperature: when a plastic can replace a metal part.

This page is technical information, not advice on standards, law or design. The standards cited in their current edition and the material manufacturers' test reports are authoritative.